Date:  12-28-2015
Number of Hours:  2.00
Manual Reference:  Chapter 5
Brief Description:  Apply BID cloth to support the stringers

Shop temperature was 25 deg C and humidity 40%.

30g resin was mixed with 11g hardner. About half of the epoxy was poured into another cup and glass bubbles were added to the original cup to create dry micro.

Dry micro was applied to the applicable corners of stringers LWX and LWY using a popsicle stick.

The BID cloth was positioned along the corners of the stringers.

36g resin and 14g hardner were mixed and combined with the excess epoxy mixed earlier.

Epoxy was applied to the BID cloth with a 1" wide paint brush.